Fraud Blocker

Wood Plastic Composite

Specifications of Kosmos & Galawood plastic wood according to Quatest 3

The following wood plastic specifications are measured at QUATEST 3 – Quality Assurance & Testing Center 3 (Quality measurement standard technical center 3). Specifically, the general warehouse Kosmos Vietnam will provide technical specifications Kosmos Wood-plastic , and Galawood Wood-plastic for you to understand more about the product and easily make the right choice.

Sample size sent to QUATEST 3
  • The Kosmos plastic wood specimen has dimensions of 2200 x 140 x 25 mm.
  • The Galawood plastic wood specimen has dimensions of 2900 x 140 x 25 mm.

Specifications indicate the moisture content of plastic wood

Kosmos Wood-plastic Galawood Wood-plastic
Moisture content methodBS EN 322: 1993BS EN 322: 1993
Result 0.4%. 0.7%.
MeaningThe moisture content of the product is only 0.4% after drying at ~103 degrees Celsius.The moisture content of the product is only 0.7% after drying at ~103 degrees Celsius.

Note: BS EN 322: 1993 is a standard of the British Standards Institution and is the English version of EN 322:1993, published by the European Commission for Standards (CEN). This International Standard specifies an oven-drying method for the determination of the moisture content of whole wood panels.

Resistant to denting of outdoor plastic wood

Kosmos Wood-plastic Galawood Wood-plastic
Indentation resistance test methodISO 24343: 2007ISO 24343: 2007
Result0.01 mm0.03 mm
MeaningThe floor only appeared a dent of about 0.01mm after placing an extremely heavy load on it.The floor only appeared a dent of about 0.03 mm after placing an extremely heavy load on it.

Note: ISO 24343 is an international standard published by the International Organization for Standardization (ISO). This International Standard describes a method for determining the residual indentation of a coating after the application and removal of a constant load.

Outdoor plastic wood has high durability
Outdoor plastic wood has high durability

Anti-fouling ability of composite wood-plastic products

Kosmos Wood-plastic Galawood Wood-plastic
Stain resistance test methodBS EN 438 – 2: 2016BS EN 438 – 2: 2016
Toothpaste stainslevel 5level 5
Coffee stainslevel 5level 5
Stains from Sodium Hydroxide 25%level 5level 5
MeaningNo visible changeNo visible change

Note: Standard EN 438-2 is a technical standard released by CEN (European Committee for Standardization), which ensures that specimens meet the standards and quality requirements during production and use.

Plastic wood surface is difficult to stain
Plastic wood surface is difficult to stain

Specific volume of plastic wood provided by Kosmos Vietnam

Kosmos Wood-plastic Galawood Wood-plastic
Specific gravityASTM D792 – 20ASTM D792 – 20
Result1.346 g / cm31.37 g / cm3
MeaningOn a volume of 1cm3, Kosmos plastic wood has a mass of 1.346 gOn a volume of 1cm3, Galawood has a mass of 1.37 g .

Note: ASTM D792-20 is an international standard that describes test methods for determining the specific gravity (density) and density of solid plastics in the form of sheets, rods, tubes or molded products.

Specifications indicate the bending strength of plastic wood

Kosmos Wood-plastic Galawood Wood-plastic
Flexural StrengthISO 178: 2010ISO 178: 2019
Result29.7 MPa34.7 MPa
MeaningKosmos plastic wood has a maximum bending strength of 29.7 MPa before breaking or being damaged.Galawood plastic wood has a maximum bending strength of 34.7 MPa before breaking or being damaged.

Note: ISO 178: 2010 & ISO 178: 2019 is a test method that indicates the flexural properties of hard and semi-rigid plastics under specified conditions.

The bending strength of plastic wood is very high
The bending strength of plastic wood is very high

Specifications indicate the tensile strength of plastic wood

Kosmos Wood-plastic Galawood Wood-plastic
Tensile StrengthASTM D638 – 14ASTM D638 – 14
Result13.0 MPa20.6 MPa
MeaningKosmos wood plastic has a maximum tensile strength of 13.0 MPa before breaking.Galawood plastic wood has a maximum tensile strength of 20.6 MPa before breaking.

Note: ASTM D638 – 14 is a standard test method for the tensile properties of plastics.

Water absorption in 24 hours of outdoor plastic wood

Kosmos Wood-plastic Galawood Wood-plastic
Water absorptionASTM D570 – 98 (2018)ASTM D570 – 98 (2018)
Result 1.16%. 1.39%.
MeaningAfter 24 hours of soaking in water, Kosmos plastic wood absorbs about 1.16% of water compared to its original weight.After 24 hours of soaking in water, Galawood plastic wood absorbs about 1.39% of water compared to its original weight.

Note: ASTM D570 – 98 (2018) is a standard test method of the International Association for Standards and Materials (ASTM) to determine the relative water absorption rates of resins when immersed in water.

Water resistance – Swelling with thickness

Kosmos Wood-plastic Galawood Wood-plastic
Thickness SwellingISO 24336: 2005ISO 24336: 2005
Result 0.1%. 0.10%.
MeaningThe swelling according to the thickness of Kosmos plastic wood after the test with water ISO 24336 : 2005 is 0.1%The swelling according to the thickness of the Galawood resin after the ISO 24336 : 2005 water test is 0.10%

Note: ISO 24336: 2005 is a test method to determine the thickness, swelling after partial immersion in water.

Dimensional change of plastic wood after moisture change

Kosmos Wood-plastic Galawood Wood-plastic
Dimensional variations in vertical direction (Longitudial direction)BS EN 13329:2016 Annex CBS EN 13329:2016 Annex C
Result0.02 mm0.1 mm
MeaningWhen the humidity changes, the size of Kosmos plastic wood will change by no more than 0.02 mm .When the humidity changes, the size of Galawood plastic wood will change by no more than 0.1 mm .

Note: BS EN 13329: 2016 is a British standard and annex C (Annex C) of this standard deals with the determination of dimensional variations after changes in humidity.

We clean plastic wood floors by spraying water.
We clean plastic wood floors by spraying water.

Wood plastic composite's ability to resist tobacco fire - Wood Plastic Composite

Kosmos Wood-plastic Galawood Wood-plastic
Resistance to cigarette burnsBS EN 438-2: 2005BS EN 438-2: 2005
ResultLevel 4Level 4
MeaningKosmos plastic wood has a slight change in the glossy finish (at certain viewing angles), or a faint scorch mark appears after testing for resistance to fire caused by cigarette butts.Galawood plastic wood has a slight change in the gloss finish (at certain viewing angles), or a faint scorch mark appears after testing for resistance to fire caused by cigarette butts.

Note: BS EN 438-2: 2005 is the standard he uses to determine the properties of high pressure decorative panels (HPL).

Wood plastic composite against fire spread
Wood plastic composite against fire spread

Formaldehyde content on Kosmos and Galawood resin wood

Kosmos Wood-plastic Galawood Wood-plastic
Formaldehyde content (Formaldehyde content)BS EN ISO 12460-5:2015BS EN ISO 12460-5:2015
Limit of detectionmg / 100gmg / 100g
ResultNot detectedNot detected
MeaningKosmos plastic wood does not emit Formaldehyde gas, does not affect health.Galawood plastic wood does not emit Formaldehyde gas, does not affect health.

Note: BS EN ISO 12460-5:2015 is an international standard for determining the amount of formaldehyde emitted from wood panels based on the extraction method (perforation method).

Outdoor plastic wood is safe for health
Outdoor plastic wood is safe for health

Kosmos and Galawood plastic wood specifications verified by Quatest 3 The above partly reflects the product quality. Because the sample size is different (based on the actual size of the product), the article is not used for comparison. If you want to know more information about the product, you can contact Kosmos Vietnam warehouse at: (+84) 903 093 221

5/5 - (70 votes)
Did this article help you?